Product introduction:
Refining agent HB-1203 for long vehicles is a synergistic mixture of multiple surfactants, which is especially suitable for desizing, scouring and bleaching processes.
Reference process:
Enzymatic desizing process (Jig dyeing machine)
Amylase M-812 1 ~ 2g / L
NaCl 2 ~ 5g / L
Scouring agent HB-1203 1 ~ 2g / L
Pad rolling (reduction rate: 100%), stacked at 70 ° C for 4 hours, and washing the supernatant of the machine at a high temperature of 90-95 ° C
wash.
Scouring Process (Rolling-Jig Dyeing Machine)
Scouring agent HB-1203 2.0-6.0g / L
NAOH 20-40 g / L
Pad rolling (reduction rate: 100%), 90 ° C-100 ° C, stacking for 2 ~ 3 hours, under high temperature conditions of 90-95 ° C
Wash on a flat washer.
Cooking process (volume steam dyeing machine)
Scouring agent HB-1203 3.0-6.0g / L
NAOH 40-60 g / L
Pad-rolling (reduction rate: 100%), steaming at 100 ° C for 1-3 minutes, on a flat washer at a high temperature of 90-95 ° C
Cleaning.
Cooking process (rope J-shaped box)
Scouring agent HB-1203 2.0-4.0g / L
NAOH 15-30 g / L
Pad rolling (reduction rate: 100%), steaming at 95 ° C-100 ° C for 1 ~ 2 hours, flattening at high temperature of 90-95 ° C
Wash on a washing machine.
Bleaching Process (Cone Dyeing Machine)
Scouring agent HB-1203 0.5-2.0g / L
35% hydrogen peroxide 3.0-6.0ml / L
Hydrogen peroxide stabilizer H-602 1.0-2.0g / L
NAOH 1.0-2.0 g / L bath ratio: 1:10, treated at 98 ° C for 45 minutes or 120 ° C for 20 minutes.
Bleaching Process (Jig Dyeing Machine)
Scouring agent HB-1203 0.5-2.0g / L
35% hydrogen peroxide 4.0-10.0ml / L
Hydrogen peroxide stabilizer H-602 2.0-4.0g / L
NAOH 1.0-2.0 g / L bath ratio: 1: 3-1: 7, 90-98 ° C treatment for 60 minutes.
Precautions:
It is recommended to make a small test when using it in the same bath with other additives.
It is mainly used for oil stain removal of polyester, nylon and its blended fabrics, the temperature range is 60-130 ℃; it can also be used for degreasing, desizing, scouring and general cleaning of other types of fabric